Corrosion Testing Standards

The test standard summaries are for general guidance only. Though believed to be accurate at the time of writing, this may change over time. So this information should not be used as a substitute for referring to a complete test standard, at an appropriate revision level.

Note: the terms salt spray, salt mist and salt fog are all in wide spread use within corrosion test standards. In this context they can be considered to be equivalent and interchangeable terms.

EN ISO 4541

金属和其他非有机涂料 – 腐蚀 (CORR) 测试

该测试涉及将含有腐蚀性盐的浆料应用于测试试样,将其暴露在高相对湿度下一段时间。

该浆料是将0.035g试剂级硝酸铜三水合物、0.165g试剂级氯化铁六水合物和1.0g试剂级氯化铵溶于50ml蒸馏水中搅拌成溶液30g水洗陶瓷级高岭土来制备的。 将该混合物施加到试样上,并放置在35°C的封闭腔室中,其暴露区在80%至90%RH之间。

有关欧洲标准(EN)的更多信息,请访问; www.cencenelec.eu