Corrosion Testing Standards

The test standard summaries are for general guidance only. Though believed to be accurate at the time of writing, this may change over time. So this information should not be used as a substitute for referring to a complete test standard, at an appropriate revision level.

Note: the terms salt spray, salt mist and salt fog are all in wide spread use within corrosion test standards. In this context they can be considered to be equivalent and interchangeable terms.

现代 CCT-D (MS600-66)

现代/起亚 CCT-D

Een versnelde corrosietest onder complexe omgevingen moet worden uitgevoerd in overeenstemming met CCT-D van MS600-66

Stap 1: Zout dippen (onderdompeling) @ 50 °C gedurende 2 uur

Stap 2: Bevochtiging @ 50°C / 95%RH gedurende 8 uur

Stap 3: Drogen bij 70°C / 30%RH gedurende 1,5 uur

Stap 4: Drogen @ 70°C / 15%RH gedurende 1,5 uur

Stap 5: 在 35°C / 100% RH gedurende 6,5 uur 时保持疲劳

Stap 6: Drogen @ 35°C / 15%RH gedurende 2 uur

Stap 7: 盐雾 @ 35°C / 95%RH gedurende 30 分钟

Stap 8: Invriezen bij -20°C gedurende 20 minuten

Overgangstijden:

Van stap 1 naar stap 2 = 30 minuten

Van stap 2 naar stap 3 = 20 minuten

Van stap 3 naar stap 4 = 20 minuten

Van stap 4 naar stap 5 = 50 minuten

Van stap 5 naar stap 6 = 50 minuten

Van stap 6 naar stap 7 = 20 minuten

Van stap 7 naar stap 8 = 60 minuten

Van stap 8 naar stap 1 = 20 minuten

De hele cyclus is 24 uur en herhaalbaar