现代 CCT-B (MS600-66)

现代/起亚 CCT-B

复杂环境下的加速腐蚀试验应按照MS600-66的CCT-B进行

步骤 1:盐雾 @ 35C / 95% RH 持续 4 小时

第 2 步:在 70C / 30%RH 下干燥 2 小时

第 3 步:在 50C / 95%RH 下润湿 2 小时

步骤 4:在 25C / 60%RH 下进行环境干燥 1.5 小时

步骤 5:在 -20C 下冷却 2.5 小时

过渡时间:

从步骤 1 到步骤 2 = 30 分钟

从步骤 2 到步骤 3 = 20 分钟

从步骤 3 到步骤 4 = 20 分钟

从步骤 4 到步骤 5 = 60 分钟

从步骤 5 到步骤 1 = 20 分钟

整个周期为12小时,可重复