马自达 MCT-3M (兆欧 601G)
马自达MES MN 601G漆膜测试方法
本测试标准的第27节讨论了腐蚀测试的5类要求
1级 – 盐雾试验
2 级 – 穿孔耐腐蚀性测试
3 级 – 耐刮擦腐蚀测试
4 级 – 边缘耐腐蚀性测试
5 级 – 丝状耐腐蚀性测试
3-4类通常被称为马自达MCT-3M,它需要一个全封闭的腔室来执行以下测试步骤:
- 1 小时盐雾 @ 35°C,符合 JIS Z 2371
- 6 小时干燥 @ 60°C / 10-30%RH
- 1 小时润湿 @ 50°C / 95% 相对湿度
测试配置文件运行 8 小时和 180 个周期
该测试可以在配有配件ACC42和ACC47的 雅诗阁循环室 中进行