Corrosion Testing Standards

The test standard summaries are for general guidance only. Though believed to be accurate at the time of writing, this may change over time. So this information should not be used as a substitute for referring to a complete test standard, at an appropriate revision level.

Note: the terms salt spray, salt mist and salt fog are all in wide spread use within corrosion test standards. In this context they can be considered to be equivalent and interchangeable terms.

Hyundai CCT-D (MS600-66)

Hyundai/Kia CCT-D

Een versnelde corrosietest onder complexe omgevingen moet worden uitgevoerd in overeenstemming met CCT-D van MS600-66

Stap 1: Zout dippen (onderdompeling) @ 50 °C gedurende 2 uurs

Stap 2: Bevochtiging @ 50°C / 95%RH gedurende 8 uurs

Stap 3: Drogen bij 70°C / 30%RH gedurende 1,5 uurs

Stap 4: Drogen @ 70°C / 15%RH gedurende 1,5 uurs

Stap 5: Bevochtiging @ 35°C / 100% RH gedurende 6,5 uurs

Stap 6: Drogen @ 35°C / 15%RH gedurende 2 uurs

Stap 7: Spray de sal @ 35°C / 95%RH gedurende 30 minuten

Stap 8: Invriezen bij -20°C gedurende 20 minuten

Overgangstijden:

Van stap 1 naar stap 2 = 30 minuten

Van stap 2 naar stap 3 = 20 minuten

Van stap 3 naar stap 4 = 20 minuten

Van stap 4 naar stap 5 = 50 minuten

Van stap 5 naar stap 6 = 50 minuten

Van stap 6 naar stap 7 = 20 minuten

Van stap 7 naar stap 8 = 60 minuten

Van stap 8 naar stap 1 = 20 minuten

De hele cyclus é 24 uur en herhaalbaar